PeñaPlast en Polvo Standard

Indoor paste in powder (thin coat)

Paste indicated to indoor places to cover surfaces of plaster or cement.
Useful life (S/ITE C1/51-L) 7 – 8 Hours
Fire resistante A1- Non combustible
Particle size 300 microns – Medium
pH (S/ITE CI/18-L) 6 – 7
Shore C Hardness (S/ITE CI/22-L) 81
Setting (S/ITE CI/50-L) More than 8 hours
Tool cleaning With water
Kg of powder used per m2 1 mm thickness 1,20 – 1,25
Kg of paste used per m2 1 mm thickness 1,65 – 1,80
Adhérence (S/Anexxe 2 NF P 74202-1 DTU 59.2)
To acrylic paint Greater than 0,5 MPa
To cement Greater than 0,5 Mpa
Density (S/ITE CI/53-L) Powder 0,97 Gr/Lt
Density (S/ITE CI/53-L) Paste 1,74 Gr/Lt
Drying time in depth (S/ITE CI/52L)
Concrete (Average thickness – 1mm coat) 4 – 5 hours
Paint (Average thickness – 1mm coat) 5 – 6 hours
Cement ( Average thickness – 1mm coat) 3 – 4 hours
Packaging 15 Kg sacks
Conservation Keep away from extreme temperatures

Knead with water at a rate of 38 to 43 percent. For each sack of 15 kg., 5,70 to 6,45 liters of water must be used for his kneading.
The knead must be manually or mechanically using an electric beater. Let the dough a few minutes, then apply. To cover with that block with cavities, a medium-sized spatula, which allows you to press firmly towards the inside of the bowl is recommended. If it is possible, to ensure that the width of the spatula is slightly greater than the size of the cavity.
The smoothing operation always vertically from top to bottom with blade, hardware and remove excess, ensuring smooth and hide all defects on surfaces. Joints are on the contrary, top to bottom. When dry, sanding and then plaster hand will be horizontally from right to left, left to right joints.
Finally, after this second hand drying, sand the surface and if there is no imperfection, go to paint on.